A liquid-cooling bellows in an AI rack carries coolant at 2.5 MPa through a wall of 0.15–0.3 mm. When one of those units leaks in the field, the tube is almost never the cause. The seam is.

0.15–0.3 mmwall at the seam
2.5 MPapressure hold + helium
0.05–50 mspulse width window

The seam is the pressure boundary

Follow the coolant on a dense AI rack. It leaves the CDU, crosses a manifold, drops into a cold plate bolted to an accelerator, and comes back. Every transition in that loop is a tolerance stack — a machined port, a quick-disconnect, a hose barb — and between them sits a short run of thin-wall stainless bellows whose job is to absorb the mismatch and the pump vibration.

The tube itself is formed, not welded, and it rarely fails. What fails is the joint at each end: a closed circle a few centimetres across, welded in a single rotation, with the head stationary and the part turning on a chuck. There is no second attempt, because the inside of that joint is the leak path — you cannot reach it after the fact without cutting the part open.

On 3 mm plate a welder has room to be approximate. On a 0.2 mm wall there is none. A 20 µm offset that nobody would notice on structural steel is a tenth of the wall here, and the beam either bridges the gap or it does not.

Four ways a seam fails, and what each one looks like

Leak testing sorts failures into a small number of repeatable signatures. Knowing which one you are looking at is what makes the parameter change obvious instead of experimental.

What the test showsWhat happenedWhat actually gets changed
Leak at one point on the circle, sharp and repeatableCrater at the start/stop overlap; the last pulse re-melted a thinned wallOverlap ratio and down-slope, not more power
Leak along the toe, heat tint running blue-goldToo much heat input; wall thinned before the seam closedPeak power, pulse width, or travel speed
Holds 0.5 MPa, leaks at 2.5 MPaRoot not fused through; a slit that only opens under loadFocus position and travel speed
Leak on one side of the circle onlySeam offset or chuck runout — the beam walked off the jointFixture, then vision alignment

Note what is missing from that table: no failure mode is fixed by turning the power up. On thin wall, the reflex of adding energy is what converts a fusion problem into a burn-through problem.

Two dials instead of one

A QCW fibre source splits heat input into two independent settings. Peak power decides whether the beam penetrates; average power decides how much the part heats up. Between them sits pulse width — from 0.05 to 50 ms — and repetition rate up to 5 kHz.

That split is the whole reason thin-wall bellows became a laser job rather than a TIG job. You can put 1,500 W of peak into a spot for a fraction of a millisecond, close the seam, and let the convolution beside it stay cool enough to keep its shape. A continuous source gives you one dial, and on 0.15 mm that dial is either too cold to fuse or hot enough to drop through.

Orbital laser welding head welding a thin-wall stainless bellows held in a rotary chuck, with the coaxial camera image on a monitor beside it
One rotation, one pass, no filler. The head stays still while the chuck turns the part; the coaxial camera holds the seam under the crosshair before the pulse train starts, so alignment is a setup step rather than something the operator corrects mid-weld.

Technical data — BWG-Q150ZD4-LY-A-545

The figures below describe the build we quote for liquid-cooling bellows in the 0.15–0.3 mm range. The four power options share one frame; what changes is the source and the head.

ParameterThis configuration
SourceQCW pulsed fibre laser, continuous output available
Peak powerQuoted per build; the bench unit shown here is a 1.5 kW-peak configuration
Average powerRoughly a tenth of peak, set by the build
Pulse width0.05–50 ms
Repetition rateup to 5 kHz
Wavelength1,070 nm
Delivery fibreCore size and length matched to the build; QBH connector; bend radius > 200 mm
Welding headLZD-D30 · 25–500 W rated · F150 collimation · 20 mm aperture · ±1.5 mm focus travel (quoted build)
Work envelope500 × 400 mm, customisable
Travel speed1–10 m/min
CoolingForced air
Supply / consumption220 V or 380 V ±5 % · 1.5 kW
FootprintFloor-standing cabinet; final dimensions confirmed on the general arrangement drawing

Configuration-dependent. Builds share the frame and the work envelope; source, head and fibre are matched to each. Check the quoted build against your drawing before ordering, and treat any figure here as a starting specification rather than a guarantee for your part.

What the machine cannot decide for you

The parameters are only half of the joint. The other half is the fixture: how the bellows is held, whether the chuck runs true, and whether the seam sits within the depth of focus across the full circle. A machine that welds perfectly on a sample will still walk off a production part that sits 50 µm off-centre in the fixture.

That is why the honest unit of sale is not the machine but the weld recipe, developed on your parts. Two suppliers can quote the same laser source and deliver different leak rates, because the fixture and the recipe are where the yield actually lives.

Where this stops being the right answer

Pulsed QCW is the default for 0.15–0.3 mm. It is not universal.

  • Wall above roughly 0.5 mm, or long straight seams. A continuous source with a stable keyhole gives a smoother bead than overlapping pulses, and heat control stops being the binding constraint.
  • Parts that are not bodies of revolution. A rotary chuck wants a circular joint. Flat or asymmetric joints need a different kinematic arrangement, not a different recipe.
  • Very low volume. Below a few hundred units a year, a skilled TIG operator with a good fixture can be the cheaper route. The laser earns its cost on repeatability at volume, not on a single perfect part.
  • Qualification regimes that require radiography or full traceability. Those are programme-level requirements; the machine can produce the weld, but the paperwork is a separate conversation and we will say so before you commit.
Finished stainless steel bellows sample with a machined tube end, welded at the transition, photographed on a work surface
A finished sample, not a rendering. Bellows run joined to a machined tube end; the weld sits in the transition where the wall steps up, which is the geometry that decides whether the joint holds 2.5 MPa.

How to verify it before you commit to a machine

Every claim in this note can be tested on your own parts, before you commit to a machine. The sequence we run with new customers:

  1. Send three parts. Three is the minimum that shows whether a result repeats; one good weld is an anecdote.
  2. We weld them and run the tests we would want run on us — helium mass-spectrometry leak detection and a 2.5 MPa pressure hold.
  3. You witness the run, or send your own tester. A leak figure you did not see measured is a number from a brochure.
  4. The recipe is frozen and written down — peak, average, pulse width, repetition rate, speed, focus, gas, overlap — so that acceptance of the machine is a comparison against a documented baseline rather than an opinion.
Close-up of the machined end of a welded bellows sample showing the bore and the weld at the tube transition
Our own trial weld, cut and photographed in the workshop. The end face tells you as much as the leak test. A clean bore with the weld confined to the shoulder means the root fused without the beam cutting into the flow path — the difference between a joint that passes today and one that still passes after a thousand thermal cycles.

43 seconds of the process above, filmed on the bench: 0.15–0.3 mm wall, 2.5 MPa, helium-verified. Watch on YouTube.

Questions buyers actually ask

What wall thickness can this weld?

0.15–0.3 mm is the standard range for the liquid-cooling bellows this note describes. Below 0.15 mm the part handling, not the laser, becomes the limit. Above 0.3 mm the pulsed source still works, but the economics shift toward a continuous build.

Is a pressure hold enough, or do I need helium?

A 2.5 MPa hold finds structural failures. Helium mass spectrometry finds the pinholes a pressure test walks past, because the leak rate that matters in a coolant loop is far below what a gauge can see. Run both; they answer different questions.

Can it weld tube to flange, not just tube to tube?

Yes. The constraint is the fixture, not the head: both ends need to be held concentric to the rotation axis, and the flange joint usually needs a dedicated clamp. We build the fixture from your CAD before delivery.

Does the heat affect the convolution next to the weld?

That is the reason for pulsed output. Average power in the 75–450 W range keeps the heat-affected zone tight enough that the convolution adjacent to the seam does not collapse. If your part shows deformation, the fix is usually pulse width and travel speed, not a different machine.

How long does a changeover take?

Once a recipe is documented, switching between two similar parts is a matter of minutes. The real cost is the fixture: a new geometry needs a new clamp, a first-article check, and a fresh baseline. That is why we ask for the drawing set early.

Send three parts and a drawing. We weld them, run the helium test and the 2.5 MPa hold, and send you the numbers with the recipe attached — whether or not you buy the machine.